Comment on First time with PETG. Is this calibration, wetness or something else?
SymbioteSynapse@lemmy.world 1 year ago
Check for a partial clog. 80% of the time i get that consistency with petg, its because the nozzle is partially clogged. The other 20% is the ptfe tubing is shot. Usually it partially melts and causes underextrusion.
Wet filament could be an issue too, but this is pretty extreme for wet filament.
drudoo@lemmy.world 1 year ago
You were right! All clogged up.
Replaced the nozzle, heat block (heating element, sensor, PTFE) and fan duct. Wasn’t able to unscrew the nozzle (got stuck 80% out) so I replaced the whole thing.
Did two new temp towers:
Left tower is 235 (top) to 260 (layers labeled 280-260 are all 260). Right is 220-240.
i.imgur.com/1MQkStE.jpg
i.imgur.com/HDWq19A.jpg